| PROPERTIES OF POLYPROPYLENE EXTRUDED RODS | ||
| Property | ASTM | Polypropylene |
| Specific Gravity | D769 | 0.902 - 0.910 |
| P.S.I. Tensile Strength | D638 | 4300 - 5500 |
| % Elongation | D638 | 200.0 - 700.0 |
| P.S.I. Comprehensive Strength | D695 | 5500 - 8000 |
| Impact strength (1/2x1/2 in. notched) | D256 | 0.5 - 2.280 (1/8 x 1/2 In bar) |
| Hardness Rockwell | D785 | 80 -110 |
| 105 P.S.I. 73 0F Flexural Modulus | D790 | 1.7 - 2.5 |
| Coefficient of friction | --- | 0.3 |
| -10 4cal sec cm3 C cm Thermal conductivity | C177 | 2.8 |
| Thermal Expansion 105 per 0C | D696 | 5.8 - 10.2 |
| Resistance to heat 0C (Continuous) | --- | 1100 C |
| Ω - cm (23 0C50%) Volume resistivity | D257 | 1016 |
| 1/8 in thickness volts mil Dielectric strength | D149 | 500-650 |
| 1 KHz Dielectric constant | D150 | 2.2 - 2.6 |
| 1 KHz Dissipation (power) factor | D150 | 0.0005 0.0018 |
| 24 / j3.2 mm% Water absorption 24 hr. 3.2 thickness, % | D570 | 0.01 - 0.03 |
| in mm Burning rate | D635 | 0.75 - 0.82 |
| Effect of weak acids | D534 | None |
| Effect of strong acids | D543 | Attacked slowly by oxidizing acids |
| Effect of weak alkalies | D543 | None |
| Effect of Strong Alkalies | D543 | Resistant |
| Effect of organic solvents | D543 | Resistant below 800 C |